304LV stainless steel

304LV stainless steel has reduced carbon content for better corrosion resistance in place of tensile strength.

 

Chemical composition

Composition

ASTM A276
UNS S30403
%

Carbon 0.03 max
Manganese 2.00 max
Phosphorus 0.045 max
Sulfur 0.030 max
Silicon 1.00 max
Chromium 18.00 - 20.00
Nickel 8.00 - 12.00
Iron Balance

 

Physical properties

  Metric

English

Density

7.29 g/cm³ 0.285 lbs/in³

Modulus of elasticity

193 GPa 28.0 Mpsi

Electrical resistivity

720
µohms*mm
28.4
µohms*in

Thermal conductivity

15.65
W/(m*°C)
9.05
BTU*in/(hr*ft²*°F)

Coefficient of linear thermal expansion

16.92
µm/(m*°C)
9.4
µin/(in*°F)

*Values calculated at 22 °C [72 °F]

 

Mechanical properties

Cold worked %

Yield strength

Ultimate tensile strength Elongation
%
0 331 MPa [48 ksi] 621 MPa [90 ksi] 40
20 562 MPa [81.5 ksi] 731 MPa [106 ksi] 27
37 800 MPa [116 ksi] 1014 MPa [147 ksi] 5.9
50 1014 MPa [147 ksi] 1193 MPa [173 ksi] 3.2
60 1151 MPa [167 ksi] 1317 MPa [191 ksi] 2.8
68 1089 MPa [158 ksi] 1420 MPa [206 ksi] 2.8
75 1262 MPa [183 ksi] 1496 MPa [217 ksi] 2.7
80 1400 MPa [203 ksi] 1538 MPa [223 ksi] 2.6
84 1455 MPa [211 ksi] 1600 MPa [232 ksi] 2.5
90 1517 MPa [220 ksi] 1655 MPa [240 ksi] 2.5
93 1710 MPa [248 ksi] 1862 MPa [270 ksi] 2.5
95 1779 MPa [258 ksi] 1937 MPa [281 ksi] 3.1

*All data represent results from 25.4 cm [10 in] test gauge length.
Values are typical and may not represent all diameters. Test method will affect results.

304LV stainless steel

304LV stainless steel has reduced carbon content for better corrosion resistance in place of tensile strength.

 

Chemical composition

Composition

ASTM A276
UNS S30403
%

Carbon 0.03 max
Manganese 2.00 max
Phosphorus 0.045 max
Sulfur 0.030 max
Silicon 1.00 max
Chromium 18.00 - 20.00
Nickel 8.00 - 12.00
Iron Balance

 

Physical properties

  Metric

English

Density

7.29 g/cm³ 0.285 lbs/in³

Modulus of elasticity

193 GPa 28.0 Mpsi

Electrical resistivity

720
µohms*mm
28.4
µohms*in

Thermal conductivity

15.65
W/(m*°C)
9.05
BTU*in/(hr*ft²*°F)

Coefficient of linear thermal expansion

16.92
µm/(m*°C)
9.4
µin/(in*°F)

*Values calculated at 22 °C [72 °F]

 

Mechanical properties

Cold worked %

Yield strength

Ultimate tensile strength Elongation
%
0 331 MPa [48 ksi] 621 MPa [90 ksi] 40
20 562 MPa [81.5 ksi] 731 MPa [106 ksi] 27
37 800 MPa [116 ksi] 1014 MPa [147 ksi] 5.9
50 1014 MPa [147 ksi] 1193 MPa [173 ksi] 3.2
60 1151 MPa [167 ksi] 1317 MPa [191 ksi] 2.8
68 1089 MPa [158 ksi] 1420 MPa [206 ksi] 2.8
75 1262 MPa [183 ksi] 1496 MPa [217 ksi] 2.7
80 1400 MPa [203 ksi] 1538 MPa [223 ksi] 2.6
84 1455 MPa [211 ksi] 1600 MPa [232 ksi] 2.5
90 1517 MPa [220 ksi] 1655 MPa [240 ksi] 2.5
93 1710 MPa [248 ksi] 1862 MPa [270 ksi] 2.5
95 1779 MPa [258 ksi] 1937 MPa [281 ksi] 3.1

*All data represent results from 25.4 cm [10 in] test gauge length.
Values are typical and may not represent all diameters. Test method will affect results.